Designing a Glove Box

Glove Box Design

Monitoring Systems | Seals and Gaskets | Permanent Seals | Non-Permanent Seals | Permeability
How does Ingression Occur? | Measuring Permeability | Permeability of Glove Box Materials


A glove box is a critical piece of equipment in many processing labs. There are several important components to consider when designing a glove box. Glove boxes need:

  1. A sufficient maintenance system to keep inert gases low.
  2. At least one clear panel to see the contents of the chamber
  3. Gloves which allow you to manipulate things inside the chamber
  4. A small, separate chamber (antechamber) allow you to bring items into and out of the glove box.

Glove boxes should be designed to reduce leakage as much as possible. Leakage can occur through:

  • Physical leaks in the system (holes, insufficient seals, etc)
  • Ingression of moisture and oxygen through glove box materials

Glove Box

Glove Box

Glove Box Monitoring Systems


An important part of designing a glove box is not just achieving inert conditions, but maintaining them. Glove boxes are designed in one of two ways to maintain low levels of moisture and oxygen over a long period of time.

  • Purge glove boxes - These regularly replace internal gas with fresh inert gas to remove contaminants.
  • Regeneration glove boxes - These systems clean internal gas with a filtration system and reintroduce it to the chamber. These glove boxes also flush the chamber with inert gas, but not as often as purge glove boxes will.

Both of these systems require constant internal monitoring of several environmental conditions (oxygen level, moisture level, internal overpressure, etc). Integrated purging software will use readings from these sensors to determine when to purge and for how long.

Whether a glove box uses a regeneration system or a purging system depends on many factors. Larger glove boxes tend to use regeneration systems to limit the amount of fresh inert gas needed to maintain them. However, these regeneration systems are complex, require regular maintenance and increase the cost of these glove boxes substantially.

The Ossila Glove Box uses a series of automated purging systems which flush the chambers with inert gases whenever oxygen, moisture, or pressure readings go beyond certain limits. There are also several purge features that can be triggered by the user to allow you to control the environment as much as possible.

Reducing Leak Points: Seals and Gaskets


Glove box leaks, seals, and sealant
Two hard surfaces with and without sealant materials.

Stationary and Permanent Seals

At the interface between two hard surfaces, there will always be a pathway for gas to pass through. On a microscopic level, the two surfaces have a high degree of roughness relative to the size of gas molecules. For this reason, a softer material is compressed between the two surfaces to fill these gaps and reduce leaks.

For stationary and permanent joins, silicone sealants can be used along with mechanical fixtures to ensure a tight fit. Alternatively, metals can be welded together to create a seamless join.

However, there are a several parts of a glove box that require non-permanent seals, such as doors for pass-throughs and feedthroughs for service lines such as power supply. For this, gaskets are extremely useful.

A gasket is a sealing component, often made of rubber or other flexible materials, used to create a tight and leak-proof connection between two or more surfaces, typically in mechanical or industrial applications. There is no permanent deformation of the materials, so these can be used to form a tight reusable seal.

Seal Type Uses in Ossila Glove Box
Permenant

Walls of glove box welded together

Walls of antechamber welded together

Non-Permenant

O-rings around glove box

Gaskets around window plates

 

Types of Gasket for Non-Permanent Seals

A gasket is a piece of material that can be placed between two surfaces to form a seal. In the context of a glove box, their main purpose is to create an air-tight seal against gas/liquids entering and leaving the system. There are many types of gasket each suited for different situations. The seals used in glove boxes are O-rings, flat gaskets, and welded permanent seals.

Flat Gaskets

Flat gaskets are used to form a seal between two surfaces as shown in the figure above. Flat gaskets can be cut to a wide variety of shapes, and they can be made from many types of materials. They are most commonly made with rubber and expanded rubber foams. Flat gaskets are often used for washers to help make seals, or rectangular joins such as windows and doors. They are especially beneficially when low clamping forces are used.

O-Rings

O-rings are doughnut-shaped mechanical gaskets that sit within a groove that is milled into one of the surfaces. These are usually made out of harder elastomeric materials such as nitrile or Viton. Compression of an O-ring creates an air-tight seal that can withstand high pressures and temperatures. These are often used in regions where high-pressure differentials occur such as inlet piping, or for the doors of vacuum chambers integrated into a glove box system.

Reducing Ingression: Permeability and Barrier Materials


The physical properties of materials used to construct a glove box will have the biggest impact on the amount of oxygen and moisture permeation that will occur. As we must keep these levels as low as possible, the choice of material is extremely important for each aspect of a laboratory glove box.

All glove boxes are slightly permeable; moisture and oxygen can pass through the walls of the glove box and enter the atmosphere inside the chamber. Ingress, in the case of glove boxes, is the diffusion of unwanted oxygen and water into a sealed chamber. Some materials are more permeable than others. For example, stainless steel and glass have much lower ingress rates than plastic. How susceptible your glove box is to contamination from the ingress of moisture and oxygen depends on the design of the glove box.

How Does Ingress Through Barrier Materials Occur?

When discussing ingress, we need to examine the permeability each material4. This is a measure of the total transport of matter through a system.4 Or in this case, the O2 or moisture through the glove box walls.

The ingress process can be split into several different steps. The figure below shows the stages of a permeant traveling through a solid barrier. First (Step 1), the vapor molecules must reach the first barrier interface, B1. Then, the permeant is absorbed at B1 (Step 2), before diffusing through the solid barrier (Step 3). The permeant then undergoes desorption at the B2 (Step 4) and diffuses away from the barrier (Step 5).

The processes in Step 2/4 are mainly determined by solubility, S, while step 3, is determined by the Diffusion coefficient, D0.

Glove box ingress: stags of permeability
The different stages that a permeant must go through to ingress through a barrier material.

Steps 2 and 4 can be described by the following adaptation of Henry’s Law:

Henry's Law

Where the Solubility, S, is determined by the partial pressure (pPM) of the permeant and Ksol is Henry’s law constant4–6. This essentially describes how quickly a permeant can be adsorbed or desorbed by the solid barrier.

The permeants movement through the solid barrier is governed by diffusion (step 3). This is often the slowest process; therefore it acts as the rate limiting step for permeability. This diffusion process can be described by Fick’s laws. Fick’s first law denotes the relationship between concentration gradient and movement of permeants across a space dx is:

Fick’s first law

Where J is the flux of permeants moving through the barrier, D is the diffusion constant, and dC/dx is the concentration difference across the barrier (from x à x+dx).

However, as permeant diffuses through a material, the concentration of the permeant at both point X and point (X+dx) will change. It is therefore necessary to consider how this process changes with time. This leads to Fick’s second law of diffusion:

Fick's second law diffusion

Where EA is the activation energy, T is temperature and R is the gas constant. This EA essentially represents the energy required for a permeant to squeeze through a solid.7 This also means ingress depends exponentially on temperature.

The permeability coefficient, P0, is a product of a systems S and D0 values. This is the property used to describe a barriers permeability to a specific permeant.

How to Measure the Permeability of Barrier Materials

Transmission rates of O2 and water vapor can be measured using a gas transmission cell.

For O2 transmission rates, a thin layer of barrier material is mounted in the center of the transmission cell to divide the two chambers11. An oxygen sensor is placed in one chamber, and this chamber is then purged with nitrogen gas to remove all O2. Meanwhile, high oxygen levels are maintained with a constant N2/O2 supply. The increase in O levels detected by the sensor as oxygen diffuses through the semi-barrier can be used to determine oxygen permeation per unit time, or the oxygen (gas) transmission rate (OTR or O2GTR).

Glove box ingress MVTR measurement
Different methods of measuring Moisture Vapor Transmission Rate. A gas transmission cell (left) can be use to measure extremely low MVTR (1. N2/O2 or N2/H2O flow; 2. N2 flow; 3. Vent to atmosphere; 4. N2 flow + H2O or O2 to Sensor). Simpler methods such as the Desiccant and Water methods (right) can be used where moisture ingress is significant.

You can also use this method to track moisture ingress. Instead of using high oxygen levels in the first chamber, use wet nitrogen. This maintains high moisture levels and you can then use an infrared sensor to detect the increase in humidity.

Another common method to measure moisture vapor transmission rates is by using the desiccant or water methods (ASTM E96). For these methods, fill a dish with either desiccant material or water and cover with a barrier film layer. Measure this dish before and after a significant period of time. In the desiccant method, you use mass gain to determine MVTR through the barrier material. In the water method, you use mass to calculate MVTR. The desiccant and water methods are much simpler to construct, but using a gas transmission cell will determine MVTR and OTR more accurately.

The units used for these measurements will vary depending on how they have been measured. Some metrics are outlined below:

  1. Moisture vapor transmission rate, MVTR, (or water vapor transmission rate, WVTR) is a measure of the rate of water passing through a film or barrier (usually per day). This is measured in g/m2/day. One way to calculate this is to measure the uptake of water via the change in mass of the material.11 However, different methods can give different values for MVTR11, so to state the conditions measured in is very important. MVTR is generally described using this equation12:
    Moisture vapour transmission rate formula
    Where P0 is the permeation constant for the barrier, p1-p2 is the partial pressure difference of water across the material, R is the ideal gas constant, EA is the activation energy and T is temperature.
  2. Moisture vapor permeability is a measure of how much moisture will penetrate a barrier per given thickness. Therefore, for this article, we will assume that MVTR ~ P0/(barrier thickness).
  3. Additionally, oxygen transmission permeability is a measure of the amount of oxygen passage through a film or barrier per day and is measured in cm3.mm/m2.day.atm.

Permeability of Various Possible Glove Box Barrier Materials

The table below lists some coefficients of oxygen and moisture permeability, and some MVTR for various materials. The footnotes detail the conditions under which these values are accurate.

Material O2. Permeability** (cm3.mm/m2.d.atm) 2O Permeability** (g.mm/m2.d.atm) MVTR (g/m2.d.atm)
PMMA 5.8-7.2 ^12,13 5.25 ^12 55.20 ***14 -
PET 1.2-2.4 ^11 0.39-0.51 ***11 -
PTFE 222 ^11 0.006 ^15 -
Silicone rubber 3940 -4330 ^11,12 1.73-3.31 ***11
Butyl rubber 7.8-85.4 0.006 ^15 -
Aluminum foil <0.006 16 - <0.01 16
Glass Coverslip(0.1-0.2mm) - - 4 x 10-6 ^^^17
Steel N/A* N/A* N/A*

*These materials behave as near “perfect barriers” for oxygen and moisture 18,19 – most of the ingression with these materials is at the joints, depends on the bonding method used or grain boundaries within the material.

**Permeability = (volume of permeant)*(film thickness) / (surface area)*(time)*(pressure drop across barrier)

***At 37°C at 90% RH

^ At 25°C at 1 atm

^^ At 20 and 40°C respectively

^^^ At 30°C at 90% RH.

Oxygen and Water Ingress Through Polymers

An early prototype of the Ossila Glove Box built using polymer plastic
An early prototype of the Ossila Glove Box built using polymer plastic; the final version uses high quality stainless steel and glass to achieve low ingress rates that are not possible with plastics.

Polymers are a popular choice for barrier materials as they are cheap, strong, and can have a wide range of material properties.

The most important thing to consider when thinking about diffusivity is the fractional free volume of the barrier material. This depends on its packing factor. Essentially, the more space there is between molecules in a barrier, the more room the gas has to diffuse through it. For this reason, permeability also depends on the size and structure of the permeant8.

Polymers consist of long chains and therefore have a low packing factor. However, whether a polymer is classed as glassy, crystalline or rubbery will affect this packing factor. Furthermore, the quality of a polymer will depend on its on its structure at room temperature. A glassy polymer has glass transition temperature, Tg>room temperature, RT, meaning that the polymer chains are locked into one position and the material will be characteristically brittle.9 A rubbery polymer will have Tg<RT, so is more malleable.

In glassy polymers, solubility is increased as they have an excess non-equilibrium free volume10. In other words, the polymers chains may be locked in awkward positions, leaving holes for moisture uptake. However, rubbery polymers tend to have a higher free volume, as they have a more disorganized structure. Also, their polymer chains have more room to move around, facilitating diffusion through the material. For this reason, rubbery polymers tend to have higher permeability.

Crystalline materials in general have a much better packing density than rubbery/glassy polymers therefore permeants have a harder time diffusing through them. When crystalline materials form, there is a point where two crystals meet. This is called a grain boundary. There can often be atomic mismatch at this grain boundary leading to slightly larger free volume, thus, there may be a small ingression of moisture or oxygen at grain boundaries7.

We use solid materials, like metal and glass, for the Ossila Glove Box, as the amount of ingression is almost negligible.

Impact of Moisture Ingress on Glove box Atmosphere

To show how the permeability of a material will result in a rise in the water content of a glove box, we have simulated how the water content inside of a glove box increases over time for different materials. We have used a wall thickness of 5mm, the values from the table above, as well as the moisture vapor transmission rate equation to model the transfer of moisture into a box with external dimensions of 60 x 60 x 50 cm in diameter.

For simplicity, it is assumed that this is a closed system at a constant temperature, with 0.01ppm of H2O in initially the system. We have also assumed that the change in concentration gradient across the walls (barriers) with time is negligible. Thus, by the time a non-negligible change in concentration gradient has occurred, the atmosphere in the glove box is already classed as compromised. Therefore, we have excluded the effect from this example. We have also considered separately the effect of ingress through rubber gloves using two common materials.

Glove box ingress moisture variation with material
Log-plot of moisture levels within a sealed box, shown in parts per million by weight (ppmW) over a period of 14 days. Inset (shown on left) show linear plot of moisture levels in ppm over 12 hours.

The resulting plots show how easily the levels of moisture can build in a closed glove box environment. In a real glove box, there would be additional purging of N2/Ar gas or atmosphere filtration, which would reduce the impact of this ingression. However, constantly purging an environment can quickly become expensive, and filtration media can become saturated - requiring frequent regeneration of the material. Therefore, when using a glove box, it is crucial to consider which materials are being used when working in this inert atmosphere.

Glove Box

Glove Box

References and Resources


Glove Box electrical feedthrough assembly Glove Box Feedthrough Assembly

Ossila laminar flow hoods are designed for effortless setup, user-friendly operation, and efficient control. This short video guide shows you how to get started with your new equipment.

Read more...
Glove Box electrical feedthrough assembly How to Choose a Lab Glove Box

There are lots of different types of glove box and they span orders of magnitude in price, so it's important to choose the best glove box for your lab.

Read more...

References


  1. Mechanism And Optimum Shape Of Knife Edge For Metal Sealing, Y. Matsuzaki et al., Trib`ol. Int., 25 (6), 397–403 (1992); DOI: 10.1016/0301-679X(92)90077-Z.
  2. A Review Of Glove Box Construction And Experimentation, C. J. Barton, (1961); DOI: 10.2172/4043015.
  3. Experimental Methods And Techniques: Basic Techniques, D. A. Vicic et al., Compr. Organomet. Chem. III, 1 197–218 (2007); DOI: 10.1016/B0-08-045047-4/00008-X.

Further Reading


An Aid to the Design of Ventilation of Radioactive areas., G. Hall et al. (2009) Nuclear Industry Guidance. Accessed at: https://www.nuclearinst.com/

Contributing Authors


Written by

Dr. Jon Griffin

Product Developer

Dr. Mary O'Kane

Application Scientist